A387 Grade 11 Class 2 is a chromium-molybdenum alloy steel plate defined in ASTM A387 and ASME SA387, used for pressure vessels and boilers that operate at elevated temperatures. The 1.25% chromium and 0.5% molybdenum composition, combined with the normalized and tempered Class 2 condition, gives the steel the strength and resistance properties that refinery equipment demands, which is why it is a standard material in hydrocrackers, reformers, and high-temperature separators.
What Is A387 Grade 11 Class 2?
The designation Grade 11 refers to the chemical composition (approximately 1.25% chromium and 0.5% molybdenum), while Class 2 refers to the heat treatment and strength level. Class 2 plates are supplied in the normalized and tempered condition and require a minimum yield strength of 310 MPa (45 ksi) and a tensile strength of 515-690 MPa (75-100 ksi), which is higher than the Class 1 level (205 MPa yield, 415-585 MPa tensile). The steel is produced in thicknesses commonly from 6 mm to 150 mm, with larger sizes available by special agreement.
Chemical Composition
Typical composition limits for A387 Grade 11 per ASTM A387/A387M are:
| Element | Range or max, % |
|---|---|
| Carbon (C) | 0.05-0.17 |
| Manganese (Mn) | 0.40-0.65 |
| Silicon (Si) | 0.50-1.00 |
| Phosphorus (P) | 0.035 max |
| Sulfur (S) | 0.035 max |
| Chromium (Cr) | 1.00-1.50 |
| Molybdenum (Mo) | 0.45-0.65 |
The mill test certificate accompanying the plates is the authoritative reference for verification.
Why Refineries Specify This Grade
High-temperature strength: the steel retains useful mechanical properties up to about 593 deg C (1100 deg F), where carbon steels lose strength rapidly.
Resistance to hydrogen attack: the chromium and molybdenum chemistry performs well in high-temperature hydrogen service, a core requirement for hydrocrackers and hydrotreaters.
Creep resistance: molybdenum improves resistance to creep deformation during long-term exposure to high temperature and pressure.
Oxidation and corrosion resistance: the chromium content provides better resistance to high-temperature oxidation than carbon steel.
Weldability with proper procedures: although welding requires strict control, the grade is routinely fabricated into large vessels with qualified procedures and post-weld heat treatment.
Applications in Refinery Service
Hydrocrackers and hydrotreating reactors.
Catalytic reformers and high-temperature process vessels.
High-pressure separators and hot hydrocarbon piping.
Heat exchangers and feed-effluent systems in refinery units.
Boiler pressure parts such as steam drums and headers.
Fabrication and Welding Requirements
Preheating: typically 150-250 deg C depending on thickness and the qualified welding procedure, to prevent hardening and cold cracking.
Interpass temperature: controlled within the procedure range, generally above the preheat minimum.
Consumables: low-hydrogen filler metals matched to the Cr-Mo composition are required.
Post-weld heat treatment: performed to relieve welding residual stresses, typically in the range of 650-700 deg C in refinery practice. The PWHT temperature must remain below the original tempering temperature of the base metal to avoid strength loss.
Testing: pressure-retaining welds are normally examined by radiographic or ultrasonic testing, with hardness checks and positive material identification where specified, and impact testing on production test coupons where required by the design code.
A387 Grade 11 Class 2 is not intended for chloride-rich marine environments, where its resistance to chloride-induced pitting and stress corrosion is limited, and it is not a low-temperature grade: for service below about -20 deg C, the impact properties must be verified against the design requirements.
Frequently Asked Questions
What is A387 Gr 11 Class 2? It is a chromium-molybdenum alloy steel plate per ASTM A387/ASME SA387 with about 1.25% chromium and 0.5% molybdenum, supplied normalized and tempered, with a minimum yield strength of 310 MPa and a tensile strength of 515-690 MPa.
What is the difference between Class 1 and Class 2? Class 2 has a higher strength level: minimum yield of 310 MPa versus 205 MPa for Class 1, and tensile of 515-690 MPa versus 415-585 MPa, achieved by the normalized and tempered heat treatment.
What is the maximum service temperature of A387 Gr 11 Class 2? commonly referenced continuous service limit is about 593 deg C (1100 deg F); above this temperature, creep and oxidation resistance decline significantly.
Why is it resistant to hydrogen attack? The chromium-molybdenum composition slows the decarburization and fissuring caused by high-temperature hydrogen, which is why the grade performs reliably in hydrocracker and hydrotreater service within the limits established by design curves.
Is post-weld heat treatment required after welding? For most pressure vessel fabrication, yes. PWHT, typically in the range of 650-700 deg C but below the tempering temperature of the base metal, relieves residual stress and restores toughness in the weld and heat-affected zone.
What are the equivalents of A387 Grade 11? The European Cr-Mo grade 13CrMo4-5 per EN 10028-2 is the closest comparable composition; ASME SA387 Grade 11 is the code designation of the same material. Equivalence must always be verified property by property against the design specification.