What GB 38CrMoAlA is
38CrMoAlA is a nitriding alloy structural steel from the Chinese GB system. Chromium and molybdenum provide hardenability through the section, while a deliberately high aluminium addition forms fine aluminium nitride particles during nitriding and produces a very hard, wear resistant case on a tough tempered core. The A suffix denotes a high quality grade with controlled residual elements and tighter limits on phosphorus and sulphur. Composition is specified in GB/T 3077 for alloy structural steels, and cold drawn bars of this grade are commonly supplied under GB/T 3078 for quality structural steel cold drawn steel.
The combination of a hard nitrided surface and a strong, dimensionally stable core is why the grade is chosen for parts that must resist sliding wear, fatigue and slight surface heating without losing shape.
Chemical composition
The table below gives the ladle analysis limits required for 38CrMoAlA under GB/T 3077. Elements shown with a maximum only are treated as residuals.
| Element | Min (%) | Max (%) |
|---|---|---|
| C | 0.35 | 0.42 |
| Si | 0.20 | 0.45 |
| Mn | 0.30 | 0.60 |
| Cr | 1.35 | 1.65 |
| Mo | 0.15 | 0.25 |
| Al | 0.70 | 1.10 |
| P | - | 0.025 |
| S | - | 0.025 |
| Ni | - | 0.30 |
| Cu | - | 0.30 |
The aluminium range is the defining feature of the grade and must be reported on the mill certificate. A low aluminium content reduces case hardness after nitriding, while an excessive addition impairs hot workability and cleanliness, so producers control the range tightly.
Mechanical properties
Mechanical requirements for 38CrMoAlA are quoted for the quenched and tempered condition on a standard test piece. Bars destined for machining are normally delivered annealed, and the annealed hardness is limited so that the material can be cut and turned economically.
| Property | Requirement |
|---|---|
| Tensile strength Rm | ≥ 980 MPa |
| Yield strength ReL | ≥ 835 MPa |
| Elongation A | ≥ 14 % |
| Reduction of area Z | ≥ 50 % |
| Charpy impact energy KU2 | ≥ 71 J |
| Delivery hardness, annealed | ≤ 229 HBW |
Physical values used for design are close to those of other low alloy steels: density about 7.85 kg/dm3 and a modulus of elasticity of roughly 206 GPa in the quenched and tempered condition.
Heat treatment and nitriding
Heat treatment determines the final combination of core strength and case hardness, and the sequence is normally carried out in three stages.
Quenching at 930 to 950 °C followed by oil cooling to develop a fully martensitic structure.
Tempering at 600 to 650 °C to obtain the required core strength and toughness, typically in the region of 250 to 300 HBW.
Nitriding at 500 to 580 °C in a gas, salt bath or plasma process, with the duration set by the required case depth.
Nitriding is a low temperature, ferritic process, so distortion remains small and no further hardening or straightening is needed afterwards. A typical case depth for gears, spindles and cylinder parts lies between 0.2 mm and 0.6 mm, and case hardness for an aluminium bearing nitriding steel usually falls in the 900 to 1100 HV range. Case depth and microstructure are verified by the methods of GB/T 11354. Nitrogen rich compound layers are kept thin for parts that must resist chipping under high contact stress.
Applications and typical parts
The grade is used where a hard, wear resistant surface is combined with a strong core and stable dimensions.
Gears, worms and worm wheels for machine tools and reducers
Extruder screws and barrels for plastics processing
Cylinder liners, cylinder barrels and piston rods for compressors
Machine tool spindles, lead screws and precision shafts
Valve stems, pump parts and high pressure fittings
Dies, forming tools and wear plates for metal forming equipment
Because the material is heat treated before final finishing, designers can machine to close tolerance first and rely on the nitriding step to add wear resistance with minimal dimension change. Typical specific pressure and sliding conditions of machine tool and hydraulic applications are well served by the hard case over a 980 MPa class core.
Ordering and quality control
State the product form and route, for example cold drawn round bar to GB/T 3078, and the delivery condition.
Specify diameter or section, length and the dimensional and straightness tolerances acceptable for automatic machining.
Require the aluminium content and the residual limits of phosphorus, sulphur, nickel and copper to be reported on the certificate.
Agree the case depth and surface hardness range, and state that case depth will be verified to GB/T 11354.
Confirm whether bars are to be supplied annealed for machining or in the quenched and tempered condition.
Decide whether ultrasonic or magnetic particle testing is required for safety related parts such as spindles and piston rods.
FAQ
Q: What does the A suffix in 38CrMoAlA mean?
It identifies the high quality variant of the grade, with controlled residual elements and tighter phosphorus and sulphur limits than a standard alloy structural steel.
Q: Which standard specifies the composition of 38CrMoAlA?
Chemical composition is specified in GB/T 3077, while cold drawn bars of the grade are commonly ordered under GB/T 3078 for quality structural steel cold drawn steel.
Q: Why is aluminium added to 38CrMoAlA?
Aluminium forms very fine nitride particles during nitriding, which is what produces the high case hardness and wear resistance of this grade.
Q: What heat treatment is used before nitriding?
Quenching from 930 to 950 °C in oil followed by tempering at 600 to 650 °C, which sets the core properties before the nitriding cycle begins.
Q: How deep is the nitrided case?
Case depth is set by time and temperature and usually falls between 0.2 mm and 0.6 mm for machine parts, verified by the methods of GB/T 11354.
Q: Can 38CrMoAlA be welded?
The high aluminium content and hardenability make welding difficult and it is normally avoided; the grade is applied to machined, nitrided parts rather than welded assemblies.