ASTM A537 Class 2 is a heat-treated carbon-manganese-silicon steel plate used primarily for fusion-welded pressure vessels, boilers, and storage tanks. The Class 2 condition means the plate is quenched and tempered for increased strength, and it is often specified for tanks built to API 650 and API 620 and for structures in the oil, gas, and petrochemical industries where higher yield and tensile strength are needed. The grade offers improved notch toughness and good weldability.
Chemical Composition
A537 Class 2 has a carbon content of about 0.24 percent maximum, manganese of 0.70 to 1.60 percent, and silicon of 0.15 to 0.50 percent. Phosphorus and sulfur are limited to 0.035 and 0.040 percent respectively. Residual elements are present in small amounts, including chromium up to about 0.25 percent, copper up to 0.35 percent, nickel up to 0.25 percent, and molybdenum up to 0.08 percent, with the balance being iron. These limits are set so that the plate can be quenched and tempered to the required strength without sacrificing weldability.
Mechanical Properties
A537 Class 2 plate has a tensile strength of 485 to 620 MPa and a minimum yield strength of 315 MPa, with a minimum elongation of 20 percent in 50 mm gauge length. The modulus of elasticity is about 200 GPa and the density is about 7.80 g per cubic centimeter, which are typical values for carbon steel. The combination of strength and toughness comes from the quenched and tempered microstructure rather than from heavy alloying.
Heat Treatment for Class 2
The Class 2 designation requires quenching and tempering. The plate is heated to the austenitizing temperature and rapidly cooled in water or oil to form a hardened microstructure, then tempered to restore toughness and ductility. This is the main difference from Class 1, which is supplied in the normalized condition. The quenched and tempered treatment produces a finer, stronger microstructure and gives Class 2 its higher yield strength.
Typical Fabrication Steps
A537 Class 2 plates are processed through a standard sequence. After receipt and verification of material certificates, the plates are cut by flame, plasma, or shearing, and the cut edges are cleaned. Forming by bending or rolling is carried out when the design requires it. Welding is performed by SMAW, GMAW, FCAW, or SAW in accordance with an approved welding procedure specification, with interpass temperature and heat input controlled to prevent embrittlement. Post-weld heat treatment is applied when required by the specification or design, typically at 595 to 650 deg C, with controlled heating and cooling rates.
Typical Applications
Fusion-welded pressure vessels and boiler shells
Storage tanks designed to API 650 and API 620
Structures and equipment in oil, gas, and petrochemical plants
Components requiring higher yield and tensile strength than normalized carbon steel
Frequently Asked Questions
What is ASTM A537 Class 2? It is a quenched and tempered carbon-manganese-silicon steel plate for fusion-welded pressure vessels and storage tanks.
What is the difference between Class 1 and Class 2? Class 1 is supplied in the normalized condition, while Class 2 is quenched and tempered for higher strength.
What is the yield strength of A537 Class 2? The minimum yield strength is 315 MPa and the tensile strength is 485 to 620 MPa.
Is A537 Class 2 weldable? Yes, it has good weldability and can be welded by SMAW, GMAW, FCAW, and SAW with an approved procedure.
When is PWHT required for A537 Class 2? Post-weld heat treatment is applied when required by the specification or design, typically at 595 to 650 deg C.
Where is A537 Class 2 used? It is used for pressure vessels, boilers, and storage tanks in the oil, gas, and petrochemical industries.