Knowledge

What type of steel is SA 387 Grade 5 Class 1?

Jan 12, 2026 Leave a message

SA 387 Grade 5 Class 1 is a chromium-molybdenum (Cr-Mo) alloy steel plate used for weldable pressure vessels and boilers operating at elevated temperatures, offering good tensile strength at high heat and improved corrosion resistance due to its alloy content. It's a robust material suited for demanding applications in the oil, gas, and power industries, characterized by specific chemical composition (around 5% Chromium, 0.4-0.7% Molybdenum) and mechanical properties that differ from Class 2.

info-439-184

Equivalents

BS EN ASME DIN
... ... SA387-5-1 ...

 

Specifications ASME SA387 Grade 5 Alloy Steel Plates

Designation Nominal Chromium
Content (%)
Nominal Molybdenum
Content (%)
SA387 Grade 5 5.00% 0.50%

 

Tensile Requirements for ASME SA387 Grade 5 Alloy Steel Plates Class 1 Plates

Designation: Requirement: Grade 5

SA387 Grade 5

Tensile strength, ksi [MPA] 75 to 100 [515 to 690]
  Yield strength, min, ksi [MPa]/(0.2% offset) 45 [310]
  Elongation in 8 in. [200mm], min % ...
  Elongation in 2 in. [50mm], min, % 18
  Reduction of area, min % 45 (measured on round specimen)
40 (measured on flat specimen)

 

Chemical Requirements for ASME SA387 Grade 5 Alloy Steel Plates

Element   Chemical Composition (%)
    SA 387 Grade 5
Carbon: Heat Analysis: 0.15 max
  Product Analysis: 0.15 max
Manganese: Heat Analysis: 0.30 - 0.60
  Product Analysis: 0.25 - 0.66
Phosphorus: Heat Analysis: 0.035
  Product Analysis: 0.035
Sulphur (max): Heat Analysis: 0.030
  Product Analysis: 0.030
Silicon: Heat Analysis: 0.50 max
  Product Analysis: 0.55 max
Chromium: Heat Analysis: 4.00 - 6.00
  Product Analysis: 3.90 - 6.10
Molybdenum: Heat Analysis: 0.45 - 0.65
  Product Analysis: 0.40 - 0.70

info-219-176

Processing Workflow of SA 387 Grade 5 Class 1

1. Material Preparation & Inspection

Manufacturing: Produced via the hot-rolled process.

Chemical Analysis: Verification of Chromium (4.00–6.00%) and Molybdenum (0.45–0.65%) content.

NDE (Non-Destructive Examination): Ultrasonic Testing (UT) per ASME SA-435 to ensure there are no internal laminar defects.

2. Cutting and Forming

Cutting: Plasma or flame cutting is used. Because Grade 5 is an air-hardening alloy, the heat-affected edges must be ground to remove the hardened layer.

Cold/Hot Forming: Class 1 material is supplied in the annealed or normalized-and-tempered condition, providing maximum ductility for rolling or bending into vessel shells.

3. Welding Process (P-No. 5A Group 1)

Preheating: Essential to prevent hydrogen-induced cracking. Preheating temperatures typically range from 300°F to 500°F (150°C to 260°C) depending on thickness.

Filler Metal: Low hydrogen electrodes (e.g., E8018-B6) are required to match the base metal chemistry.

Interpass Temperature: Must be strictly controlled (usually maintained below 600°F/315°C).

4. Heat Treatment (Crucial Step)

Class 1 status requires specific mechanical properties (Tensile Strength: 60-85 ksi / 415-585 MPa).

Annealing: Heating to the critical range and cooling slowly in the furnace.

Normalizing & Tempering:

Normalizing: Air cooling from above the transformation temperature.

Tempering: Must be performed at a minimum temperature of 1300°F (705°C) to ensure the material reaches the Class 1 ductile state.

5. Post-Weld Heat Treatment (PWHT)

Mandatory for SA 387 Grade 5.

The assembly is held at approximately 1300°F - 1400°F (705°C - 760°C) to relieve residual stresses and improve the toughness of the weld zones.

6. Final Testing & Certification

Mechanical Testing: Tensile, Yield, and Elongation tests.

Impact Testing: Charpy V-notch tests if required by the specific pressure vessel design code (e.g., ASME Section VIII).

Final NDT: Magnetic Particle (MT) or Radiographic Testing (RT) of all weld seams.

 

Applications

Pressure Vessels: For containing pressurized gases and liquids at elevated temperatures.

Boilers & Heat Exchangers: In power plants and petrochemical facilities for efficient heat transfer.

Oil & Gas Industry: In refineries, offshore rigs, and pipelines for sour service (sulfide stress cracking) resistance.

Storage Tanks: For storing high-temperature liquids and gases.

Industrial Equipment: Found in various heavy-duty construction and processing equipment.

 

Advantages

High Temperature Strength: Maintains tensile strength at high temperatures.

Corrosion & Oxidation Resistance: Added chromium and molybdenum provide excellent resistance in harsh chemical and acidic environments.

Weldability: Low carbon content and balanced composition allow for easy welding without cracking.

Durability & Longevity: Resists abrasion, corrosion, and stress, leading to longer service life and lower maintenance.

Cost-Effective: Long-term savings due to reduced maintenance and extended service life often outweigh the initial material cost.

Versatility: Suitable for diverse applications requiring strength, heat resistance, and corrosion protection.

Contact now

For more details about GNEE's steel products, contact us at beam@gneesteelgroup.com. We look forward to working with you.

 

Does SA 387 Grade 5 Class 1 require preheating before welding?

Preheating is often recommended, especially for thicker plates or in cold environments, to reduce the risk of hydrogen-induced cracking and ensure sound welds.

 

What post-weld heat treatment is typically applied to SA 387 Grade 5 Class 1?

Stress relief heat treatment is commonly applied after welding to reduce residual stresses and improve the material's toughness and dimensional stability.

 

What industries commonly use SA 387 Grade 5 Class 1?

It is widely used in the oil and gas, petrochemical, chemical processing, and power generation industries.

 

What types of equipment are often made from SA 387 Grade 5 Class 1?

Typical applications include pressure vessels, boilers, heat exchangers, and other pressure-containing components.

 

At what temperature range is SA 387 Grade 5 Class 1 typically used?

It is designed for service at moderate to elevated temperatures, where both pressure and temperature place significant demands on the material.

 

How does SA 387 Grade 5 Class 1 compare to other grades in the SA 387 series?

Compared to higher-strength grades in the SA 387 series, Grade 5 offers moderate strength with good toughness and weldability, making it suitable for less severe service conditions.

 

What is the chemical composition focus of SA 387 Grade 5 Class 1?

Its composition is balanced with moderate carbon and manganese content to provide strength and toughness, while limiting impurities to ensure good weldability and resistance to brittle fracture.

 

What testing is typically performed on SA 387 Grade 5 Class 1 plates?

Common tests include tensile testing, impact testing (such as Charpy V-notch), bend testing, and ultrasonic examination to ensure material quality and performance.

 

What is the significance of notch toughness in SA 387 Grade 5 Class 1?

Notch toughness is important because it helps the material resist brittle fracture, which is critical in pressure vessels where sudden failure could have severe consequences.

 

What should be considered when selecting SA 387 Grade 5 Class 1 for a project?

Key considerations include the operating temperature and pressure, thickness of the plates, welding procedures, required toughness, and any specific code or purchaser requirements for heat treatment and testing.

Send Inquiry