Two Different Chinese Standards, Two Strength Classes
Q235 and Q345 belong to different Chinese standards and different strength classes. Q235 is a carbon structural steel defined by GB/T 700-2006, in which the number states the minimum yield strength in MPa. Q345 was the low-alloy high-strength grade of GB/T 1591. When GB/T 1591-2018 was implemented on 1 February 2019, the Q345 designation was replaced by Q355, whose strength level matches the European S355 grade. On current drawings the correct designation is Q355, and Q345 should be read as the older equivalent.
The letter Q stands for yield in Chinese practice, so the grade number is a yield-strength promise rather than a tensile-strength promise. That single convention explains most of the confusion when Chinese grades are compared with Japanese SS grades, where the number refers to tensile strength.
Chemical Composition and What Drives the Difference
| Element (max unless noted) | Q235B, GB/T 700-2006 | Q355B, GB/T 1591-2018 |
|---|---|---|
| Carbon | 0.20 % | 0.20 % |
| Silicon | 0.35 % | 0.55 % |
| Manganese | 1.40 % | 1.60 % |
| Phosphorus | 0.035 % | 0.035 % |
| Sulphur | 0.035 % | 0.035 % |
Q355 carries a deliberate manganese addition plus microalloying elements such as niobium, vanadium or titanium, which refine the grain and raise yield strength without raising carbon. That is why Q355 keeps good weldability at a 355 MPa yield level, and why its carbon equivalent, not its carbon content, is the number a welding engineer must check before fabrication.
Mechanical Properties Compared
| Property | Q235B | Q355B | Q355D |
|---|---|---|---|
| Minimum yield strength, t ≤ 16 mm | 235 MPa | 355 MPa | 355 MPa |
| Tensile strength | 370-500 MPa | 470-630 MPa | 470-630 MPa |
| Minimum elongation | 26 % | 22 % | 22 % |
| Charpy impact test | 27 J at +20 °C | 34 J at +20 °C | 34 J at -20 °C |
The yield step from 235 to 355 MPa is a gain of about 50 % in load capacity for the same section. Ductility falls slightly, from a 26 % minimum elongation to 22 %, which remains adequate for static building frames but must be considered in seismic detailing. Yield strength also falls as thickness rises in both standards, so the value must be taken at the thickness actually ordered.
Choosing Between Them
Q235B remains the economical default for light framing, secondary members, platforms, handrails and general fabrication, and it is easier to bend and weld in simple workshops. Q355 becomes the better choice once member sizes are driving the design: long-span beams, heavily loaded columns, crane girders, and structures where reducing self-weight also reduces foundation cost. In low-temperature service the quality suffix matters more than the strength class, and Q355D with its -20 °C impact requirement is a common specification for cold-climate projects.
Mixing the Two on One Project
Mixed-grade fabrication is normal, but the two steels must be identified separately throughout the shop. Use grade stamps or colour coding, keep separate mill certificates, and do not allow a welding procedure qualified on Q235B to be applied to Q355 without checking the carbon equivalent and the consumable selection. Where dissimilar thicknesses are welded, preheat requirements are set by the thicker component.
Frequently Asked Questions
Q: Is Q345 the same as Q355?
A: Functionally yes for most purposes. GB/T 1591-2018 replaced Q345 with Q355 from 1 February 2019, and the new grade matches the European S355 strength level.
Q: How much stronger is Q355 than Q235?
A: The minimum yield strength is 355 MPa against 235 MPa, an increase of about 50 %. Tensile strength rises from 370-500 MPa to 470-630 MPa.
Q: Can Q235 and Q355 be welded to each other?
A: Yes, with a welding procedure qualified for the higher-strength grade. The controlling parameters are the carbon equivalent of Q355 and the thickness of the thicker part.
Q: Which grade is better for cold climates?
A: The grade family matters less than the quality suffix. Q355D guarantees 34 J at -20 °C, whereas Q235B is only impact tested at +20 °C.
Q: Does the price difference justify Q355?
A: Only when the higher yield strength removes steel. If a Q235B section already satisfies the design, the premium for Q355 buys no benefit.