15CrMoR is a chromium-molybdenum steel plate for boilers and pressure vessels, standardised in GB/T 713, the Chinese standard for steel plates used in pressure equipment. The R in the designation identifies the material as a vessel grade. Its roughly 1.25 % chromium and 0.5 % molybdenum make it a member of the same metallurgical family as the 1.25Cr-0.5Mo steels covered internationally by ASTM A387/A387M Grade 11, and that composition is what allows the steel to be used at wall temperatures where plain carbon steel would lose strength or suffer internal attack.
Composition and Mechanical Basis
| Item | Typical specification value |
|---|---|
| Carbon | 0.12-0.18 % |
| Silicon | 0.15-0.40 % |
| Manganese | 0.40-0.70 % |
| Chromium | 0.80-1.20 % |
| Molybdenum | 0.45-0.60 % |
| Phosphorus, maximum | 0.025 % |
| Sulfur, maximum | 0.010 % |
| Tensile strength | 450-590 MPa |
| Minimum yield strength | 275 MPa |
| Elongation | Typically not less than 19 %, tabulated in GB/T 713 by thickness |
| Heat treatment | Normalised and tempered, with impact requirements stated by thickness |
The balance of chromium and molybdenum does three jobs at once. It raises the elevated-temperature yield and creep strength so that a thinner wall can be used at design metal temperatures that commonly reach about 550 degC; it improves resistance to oxidation and to the aggressive service environments found in refining and chemical plant; and, crucially, it raises the temperature at which hydrogen at partial pressure can attack the steel. The carbon content is deliberately modest so that the plate can be welded and post-weld heat treated without excessive hardening, and sulfur is held very low to control inclusion shape and through-thickness ductility.
Applications in the Power and Process Industries
| Application | Why the grade fits |
|---|---|
| Boiler steam drums and shells | Elevated-temperature strength and creep resistance at drum wall temperatures above carbon steel limits |
| Superheater and reheater headers, steam piping components | Retains strength where steam temperature is high, with predictable creep behaviour |
| Hydrotreating, hydrocracking and desulfurisation reactors | Resistance to high-temperature hydrogen attack, evaluated against the service curves used for hydrogen service |
| Heat exchangers and air coolers in refinery and chemical service | Combination of strength, oxidation resistance and weldability in the normalised and tempered condition |
| Coal chemical and fertiliser plant equipment | Service in gasification, shift conversion and ammonia plant piping and vessels at elevated temperature |
| Storage and process vessels in the pharmaceutical and fine chemical sector | Consistent mechanical properties and good weldability for pressure equipment fabrication |
For hydrogen service the decisive question is not mechanical strength but resistance to high-temperature hydrogen attack, where hydrogen diffuses into the steel and reacts with carbon to form methane at grain boundaries, causing internal decarburisation and fissuring. Selection is made against the recognised hydrogen service curves published for refinery and petrochemical equipment, such as those given in API RP 941, which relate hydrogen partial pressure and temperature to the acceptable steel family. 15CrMoR sits in the Cr-Mo range that remains acceptable to higher temperatures and pressures than carbon steel, but the operating envelope must still be checked for each case rather than assumed from the plate grade.
Fabrication, Heat Treatment and Inspection
Plates are normally delivered in the normalised and tempered condition, with typical practice using a normalising treatment in the region of 900 degC to 930 degC followed by tempering in the range of about 630 degC to 680 degC, and the exact cycle recorded on the mill certificate. Welding is carried out with matching chromium-molybdenum consumables, with preheat applied to control hydrogen cracking in the heat-affected zone and with interpass temperature kept inside the qualified range. Post-weld heat treatment is not optional for this family of steels: it relieves residual stress, tempers the hardened weld zone and restores toughness, and where thick sections are used in hydrogen service the specification also places limits on the embrittlement-related composition parameters that must be verified from the heat analysis. Welding procedures are qualified to the applicable pressure equipment standards, and non-destructive examination of plate and welds is performed by ultrasonic and radiographic methods to the relevant level of acceptance, with ultrasonic examination of plate used to exclude laminations and internal discontinuities before fabrication begins.
Properties That Must Be Checked Before Ordering
A purchase specification for 15CrMoR should state the plate thickness and the resulting mechanical property table, the heat treatment condition required on delivery, the impact test temperature and energy, the maximum carbon equivalent or embrittlement parameters if the equipment is in hydrogen or thick-wall service, the ultrasonic acceptance level for the plate, and the inspection documents to be supplied. Because the elevated-temperature design allowable stresses depend on the exact grade and condition, the design office rather than the supplier should confirm that the delivered plate is acceptable for the intended metal temperature, and any change of heat treatment made to suit welding should be reviewed against that design assumption.
Frequently Asked Questions
Q: What kind of steel is 15CrMoR?
A: It is a chromium-molybdenum pressure vessel plate covered by GB/T 713, containing about 1.25 % chromium and 0.5 % molybdenum, belonging to the same family as the 1.25Cr-0.5Mo grades of ASTM A387/A387M Grade 11.
Q: Up to what temperature is 15CrMoR normally used?
A: Design metal temperatures commonly reach about 550 degC, the exact allowable stress being taken from the design standard for the grade and thickness rather than from the material name alone.
Q: Why is post-weld heat treatment required?
A: Welding creates hard, stressed microstructures in the heat-affected zone of a Cr-Mo steel. Post-weld heat treatment relieves stress, tempers those zones and restores toughness, and is required for pressure equipment fabricated from this grade.
Q: What governs its use in hydrogen service?
A: Resistance to high-temperature hydrogen attack, assessed against the recognised hydrogen service curves such as those in API RP 941, using the hydrogen partial pressure and metal temperature of the actual operation.
Q: How is the plate inspected?
A: The plate is normally supplied in the normalised and tempered condition with a mill certificate showing composition and mechanical results, and ultrasonic examination to a specified acceptance level is used to exclude internal discontinuities before fabrication.
Q: Can 15CrMoR be welded to carbon steel?
A: Dissimilar joints are made with consumables and procedures chosen for the combination, with preheat and post-weld heat treatment set by the thicker or more highly alloyed component; the joint must be qualified in its own right.