Product Overview
HEB 160 is a European wide flange I section produced by hot rolling from weldable fine grain structural steel. Nominal section data: height 160 mm, flange width 160 mm, web thickness 8 mm, flange thickness 13 mm, root radius 15 mm, cross sectional area about 54.3 cm2 and mass about 42.6 kg per metre. The section is supplied in two low temperature grades with the same nominal strength class: S355NL rolled to EN 10025-3 and S355ML rolled to EN 10025-4. Both are qualified with a minimum Charpy V notch energy of 27 J at minus 50°C.
Section Data and Dimensional Standards
| Parameter | HEB 160 nominal value | Remarks |
|---|---|---|
| Section height h | 160 mm | Parallel flange |
| Flange width b | 160 mm | Symmetrical section |
| Web thickness tw | 8 mm | Nominal |
| Flange thickness tf | 13 mm | Nominal |
| Root radius r | 15 mm | Nominal |
| Cross sectional area | about 54.3 cm2 | Nominal |
| Mass per metre | about 42.6 kg/m | Nominal |
| Shape dimensions | EN 10365 | Tolerances to EN 10034 |
When the section is ordered by its nominal designation, the enquiry should state whether normal or tight dimensional tolerances apply, because flange thickness, out of square and straightness limits for hot rolled I and H sections are governed by the dimensional standard rather than by the steel grade standard.
Chemical Composition
The figures below are maximum values from heat analysis; product analysis allows the small deviations defined in each standard.
| Element, % | S355NL, EN 10025-3 | S355ML, EN 10025-4 |
|---|---|---|
| C | 0.18 max | 0.14 max |
| Si | 0.50 max | 0.50 max |
| Mn | 0.90 - 1.65 | 1.60 max |
| P | 0.025 max | 0.025 max |
| S | 0.020 max | 0.020 max |
| N | 0.015 max | 0.015 max |
| Al total | 0.020 min | Not a requirement of the delivery condition |
The lower carbon ceiling of S355ML follows from the thermomechanical rolling route: grain refinement and toughness are produced by controlled rolling instead of a normalising treatment, so the grade can be used for long products that cannot be re-heat treated after rolling. Niobium, vanadium and titanium are permitted within the limits of the standard to support grain refinement, and the low carbon level reduces hardening in the heat affected zone.
Mechanical Properties
| Property | S355NL | S355ML |
|---|---|---|
| Minimum yield strength, thickness up to 16 mm | 355 MPa | 355 MPa |
| Minimum yield strength, above 16 mm up to 40 mm | 345 MPa | 345 MPa |
| Tensile strength | 470 - 630 MPa | 450 - 600 MPa |
| Minimum elongation | 22 % | 22 % |
| Charpy V notch energy | 27 J at minus 50°C | 27 J at minus 50°C |
Yield strength is specified in thickness steps, so a section or plate is entitled to the 355 MPa value only inside the first thickness bracket. Tensile testing is normally performed per heat or per test unit, and a 3.1 inspection document to EN 10204 is the usual basis for structural acceptance.
Selection Notes for Cold Climate Projects
At service temperatures close to minus 50°C both grades meet the toughness requirement, so the choice depends on how the component is manufactured. S355NL suits components that are normalised, or stress relieved after forming, such as welded box sections and heavy built up girders. S355ML suits long rolled products that cannot be post weld normalised, and its lower carbon content tolerates a wider welding window. Where impact testing of the finished component at the design temperature is required, the test has to be ordered separately, because the standard value relates to the delivery condition of the steel.
Applications
Typical uses include wind turbine towers and foundations, offshore platform secondary structures, bridge girders and bearings, crane runways, cold climate building frames and heavy transport equipment. Because the wide flange spreads load evenly and raises bending and shear capacity for a given mass, the HEB 160 section is often chosen where stiffness rather than strength governs the design.
Frequently Asked Questions
Q: What is the difference between S355NL and S355ML?
A: S355NL is normalised or normalised rolled to EN 10025-3 with a maximum carbon content of 0.18 %. S355ML is thermomechanically rolled to EN 10025-4 with a maximum carbon content of 0.14 %, so it obtains toughness and grain refinement from controlled rolling rather than from heat treatment.
Q: What does the letter L mean in S355NL and S355ML?
A: It stands for a minimum Charpy V notch impact energy of 27 J tested at minus 50°C. Grades carrying the suffix N have the same energy requirement at minus 20°C.
Q: What is the mass of HEB 160 per metre?
A: About 42.6 kg/m for the nominal section, with a cross sectional area of about 54.3 cm2.
Q: Can S355ML be normalised after rolling?
A: Normalising would remove the thermomechanical condition on which the grade is based. If post forming heat treatment is planned, S355NL is the appropriate selection.
Q: Is 355 MPa the yield strength at every thickness?
A: No. The 355 MPa minimum applies to nominal thickness up to 16 mm; from above 16 mm to 40 mm the specified minimum is 345 MPa, and the standard continues to step the value down at greater thicknesses.
Q: What documents are supplied with the material?
A: Mill test certificates to EN 10204 3.1 are normally issued, covering heat analysis, tensile results and impact results for the tested unit, and third party inspection can be arranged on request.