Overview of ASTM A572 High-Strength Steel I Beams
ASTM A572/A572M covers high-strength low-alloy (HSLA) columbium-vanadium structural steel in five grades: 42, 50, 55, 60 and 65. The figure after the dash is the minimum yield point in ksi, so an "A572-50" I beam is certified to a minimum yield point of 50 ksi [345 MPa]. Grade 50 develops roughly 39% more yield strength than general structural carbon steel to ASTM A36, which is why hot-rolled I beams, universal beams and wide-flange sections in building frames, mezzanines, pipe racks and equipment supports are increasingly ordered in A572 Grade 50 instead of A36. The low columbium and vanadium additions also refine grain size, which raises strength and improves atmospheric corrosion behaviour without the cost of a fully alloyed steel.
Heat Analysis Limits by Grade
Table 1 lists the heat analysis limits laid down in the specification for the three grades most commonly rolled as beams. Phosphorus is limited to 0.04% max and sulfur to 0.05% max in all of them; larger limits than heat analysis apply to product analysis, as defined in the standard.
| Grade | C max, % | Mn max, % | Si max, % |
|---|---|---|---|
| 42 | 0.21 | 1.35 | 0.40 |
| 50 | 0.23 | 1.35 | 0.40 |
| 55 | 0.25 | 1.35 | 0.40 |
Minimum Tensile Requirements
Tensile requirements are stated separately for plates and bars and for shapes. The values in Table 2 are the minimum yield point and the minimum tensile strength for the same three grades.
| Grade | Yield point min, ksi [MPa] | Tensile strength min, ksi [MPa] |
|---|---|---|
| 42 | 42 [290] | 60 [415] |
| 50 | 50 [345] | 65 [450] |
| 55 | 55 [380] | 70 [485] |
Grades 60 and 65 are also available at 60 ksi [415 MPa] and 65 ksi [450 MPa] minimum yield. Plates in those two grades are restricted to a maximum thickness of 1.5 in. [40 mm], whereas Grade 50 plates and bars are covered up to 6 in. [150 mm]. Thickness limits are worth checking before a section list is frozen, because the permitted heat analysis is tied to the product form and thickness range.
Hot-Rolled I Sections Rolled in A572 Grade 50
I beams with parallel flanges are rolled to nominal dimensions given in EN 10365 and are routinely produced in A572 Grade 50 material, which allows a European shape to be married to an ASTM material certificate. Table 3 shows a representative part of the IPE range.
| Section | Depth, mm | Width, mm | Web, mm | Flange, mm | Mass, kg/m |
|---|---|---|---|---|---|
| IPE 100 | 100 | 55 | 4.1 | 5.7 | 8.1 |
| IPE 140 | 140 | 73 | 4.7 | 6.9 | 12.9 |
| IPE 180 | 180 | 91 | 5.3 | 8.0 | 18.8 |
| IPE 220 | 220 | 110 | 5.9 | 9.2 | 26.2 |
| IPE 270 | 270 | 135 | 6.6 | 10.2 | 36.1 |
| IPE 300 | 300 | 150 | 7.1 | 10.7 | 42.2 |
Fabrication and Purchasing Notes
The carbon equivalent is not controlled by ASTM A572, so welding procedure qualification should be based on the carbon equivalent calculated from the heat analysis printed on the mill certificate, with preheat selected from AWS D1.1 for the thickness involved. Beams are normally supplied hot rolled, shot blasted and either black, primed or galvanised, in random or fixed lengths, and tolerances on depth, out-of-square and camber follow ASTM A6/A6M. For buying purposes, state the specification, grade, section designation, length, surface condition and whether a plate or shape tensile test is required, because A572 sets different tensile requirements for the two product forms.
Frequently Asked Questions
Q: What is the minimum yield strength of ASTM A572 Grade 50 steel?
A: 50 ksi [345 MPa] minimum yield point, with a minimum tensile strength of 65 ksi [450 MPa].
Q: Is A572 Grade 50 the same as ASTM A992?
A: No. A992 applies only to structural shapes and adds a yield range of 50 to 65 ksi, a maximum yield-to-tensile ratio of 0.85, a carbon equivalent limit of 0.45% and a Charpy V-notch minimum of 20 ft-lbf [27 J] at 70 F [21 C].
Q: Can A572 Grade 50 beams be welded without preheat?
A: The specification itself does not require preheat, but preheat is generally selected from AWS D1.1 as a function of thickness and the carbon equivalent computed from the certified chemistry.
Q: How thick can A572 Grade 50 material be supplied?
A: Plates and bars are covered to 6 in. [150 mm] maximum thickness for Grade 50; Grade 60 and Grade 65 plates are limited to 1.5 in. [40 mm].
Q: Does A572 Grade 50 resist atmospheric corrosion?
A: The columbium and vanadium present improve grain refinement and may slightly improve atmospheric performance, but the steel is not a weathering grade. Unpainted weathering service is specified under ASTM A588/A588M, which controls copper, chromium and nickel contents.
Q: What does A572-50 mean on a mill certificate?
A: It is the industry shorthand for ASTM A572/A572M Grade 50, indicating the minimum yield point of 50 ksi.