P275NH is a weldable fine-grain steel categorized under the European standard EN 10028-3. It is primarily used for manufacturing boilers, pressure vessels, and pipes conveying hot liquids, specifically designed for moderate to high-temperature services

|
P275NH Chemical Composition |
|||||||
|
Grade |
The Element Max (%) |
||||||
|
C |
Si |
Mn |
P |
S |
Al(min) |
N |
|
|
P275NH |
0.16 |
0.40 |
0.5-1.40 |
0.030 |
0.020 |
|
0.02 |
|
Cr |
Cu |
Mo |
Nb |
Ni |
Ti |
V |
|
|
0.30 |
0.30 |
0.08 |
0.005 |
0.50 |
0.03 |
0.05 |
|
|
Grade |
|
P275NH Mechanical Property |
|||||
|
Thickness |
Yield |
Tensilmie |
Elongation |
Impact Energy(KV J) min |
|||
|
P275NH |
mm |
Min Mpa |
Mpa |
Min % |
-20° |
0° |
+20° |
|
≤ 16 |
275 |
390-510 |
24 |
47 |
55 |
63 |
|
|
16> to ≤35 |
275 |
390-510 |
24 |
47 |
55 |
63 |
|
|
35> to ≤50 |
265 |
390-510 |
24 |
47 |
55 |
63 |
|
|
50> to ≤70 |
255 |
390-510 |
24 |
47 |
55 |
63 |
|
|
70> to ≤100 |
235 |
370-490 |
23 |
47 |
55 |
63 |
|
|
100> to ≤150 |
235 |
350-470 |
23 |
47 |
55 |
63 |
|
|
Equivalent steel grade of P275NH |
|||||||
|
Europe |
Belgium |
Germany |
BS 1501 |
Italy |
ASTM |
India |
Japan |
|
|
|
WSt E285 |
224 Gr. 430 |
|
A516 Gr. 60 |
|
|
Processes Adopted for P275NH
Normalization Heat Treatment:It is a mandatory core process adopted for P275NH. The material is heated to 890-950℃, held at this temperature for a sufficient time to ensure uniform heating, then cooled in air. This process refines the grain structure, enhances toughness and mechanical stability, and guarantees the material meets the required yield strength (≥275MPa) for high-temperature and pressure service.
Forming Processes:Cold forming and hot forming are mainly adopted. Cold forming (bending, stamping, rolling) is conducted at room temperature with appropriate forming force, suitable for simple-shaped components. Hot forming is adopted for complex parts (e.g., boiler drums), with heating to 700-1050℃ to improve plasticity, followed by necessary stress relief treatment to eliminate residual stress.
Welding Processes:Commonly adopted welding processes include Shielded Metal Arc Welding (SMAW), Gas Metal Arc Welding (GMAW), and Gas Tungsten Arc Welding (GTAW). Preheating (80-150℃, adjusted by material thickness) is performed before welding, and post-weld heat treatment (550-650℃) is applied to optimize joint performance and avoid welding cracks.
Finishing and Inspection Processes:Post-processing adopts grinding and deburring to remove surface defects. Ultrasonic inspection is strictly adopted in accordance with EN 10028-3 standard to detect internal flaws (e.g., cracks, inclusions). Surface cleaning (shot blasting, pickling) is also adopted as needed to ensure product quality meets industrial application requirements.
Key Applications
Boiler and Pressure Vessel Manufacturing:As a core material under EN 10028-3 standard, it is mainly used to make boiler drums, high-pressure reactors, heat exchangers and liquid storage tanks. It is suitable for equipment operating in high-temperature environments, ensuring safe operation under pressure and thermal load .
Petrochemical Industry:Widely applied in the production of storage tanks, separators, and pipeline components (flanges, valves) for oil and gas processing. It can resist corrosion from mediums and adapt to harsh working conditions in petrochemical plants .
Power Industry:Used to manufacture key components such as high-pressure water pipes of hydropower stations and thermal power generation equipment. Its excellent high-temperature stability meets the long-term operation needs of power equipment .
Other Fields:Applied in bridge structures, high-rise building frames, and ship hull structures due to high strength. Also used in food industry high-temperature cooking equipment and nuclear reactor pressure shells .
advantages
1. High-Temperature Performance
Thermal Stability: It is specifically designed for moderate to high-temperature services.
Creep Resistance: The "NH" designation indicates specified elevated temperature properties, ensuring the material maintains its structural integrity and mechanical strength when exposed to heat.
2. Excellent Weldability
Ease of Fabrication: As a weldable fine-grain steel, it is highly compatible with standard welding processes (such as SAW or manual welding) without the risk of significant brittle cracking.
Uniformity: The normalized delivery condition ensures a consistent internal structure, which simplifies the welding and forming processes.
3. Superior Toughness and Ductility
Impact Resistance: It possesses excellent toughness even at lower temperatures, typically meeting impact test requirements at -20°C or above.
Deformation Capacity: Good ductility allows the steel to deform under high stress rather than fracturing abruptly, a critical safety feature for containing pressurized gases or chemicals.
4. Structural Integrity
High Strength: With a minimum yield strength of 275 MPa, it can bear substantial loads without permanent deformation.
Reliability: For added safety, these plates often undergo ultrasonic examination after rolling to ensure there are no internal defects before they are used in high-pressure environments.
5. Versatile Processing
Forming Capabilities: It demonstrates good cold and hot-rolling properties, making it easier for manufacturers to shape into cylinders, spheres, or complex pipe fittings.
Secondary Services: The material is well-suited for additional processing like CNC machining, beveling, drilling, and plasma cutting.
If you have project requirements for P275NH, we welcome your inquiry. GNEE maintains a large inventory of commonly used high strength steel grades for your selection.For detailed mechanical properties, chemical composition, and technical data, as well as free samples, please contact our factory immediately. We offer competitive prices, stable quality, and professional service. Email:beam@gneesteelgroup.com.
What is the thermal conductivity of P275NH?
The thermal conductivity of P275NH is about 45 W/(m·K) at room temperature. This good thermal conductivity makes it suitable for heat exchanger and boiler applications where heat transfer efficiency is important.
What welding consumables are recommended for P275NH?
Recommended welding consumables: manual arc welding uses E43XX or E50XX electrodes, gas metal arc welding uses ER70S-6 wires, and submerged arc welding uses H08MnA wires with SJ101 fluxes, matching the base metal's properties.
What is the elongation requirement of P275NH?
P275NH has a minimum elongation of 24% (for gauge length 50mm). This high elongation ensures good ductility, allowing the material to deform plastically without fracture under load or pressure fluctuations.
Can P275NH be machined easily?
Yes, P275NH has good machinability due to its moderate hardness and fine-grain structure. Ordinary cutting tools can be used, with proper cutting speed and feed rate to achieve high machining accuracy and surface quality.
What is the weight per square meter of a P275NH plate with 10mm thickness?
The density of P275NH is 7.85 g/cm³. A 10mm thick plate weighs 78.5 kg per square meter (calculation: 10mm × 7.85 g/cm³ × 100cm × 100cm / 1000 = 78.5 kg).
What certificates are required for P275NH supply?
Supply certificates for P275NH include EN 10204 3.1 or 3.2 certificates, which confirm compliance with standard requirements. They include chemical composition, mechanical properties, heat treatment, and inspection results.
What is the hardness range of P275NH after normalizing?
After normalizing, P275NH has a Brinell hardness (HB) range of 110-170. This moderate hardness balances strength and toughness, facilitating machining and welding operations.
Can P275NH be subjected to post-weld heat treatment (PWHT)?
Yes, PWHT is feasible for P275NH, typically at 550-650°C for stress relief. It reduces welding residual stresses, improves material toughness, and minimizes the risk of cracking in pressure vessel service.
What are the inspection methods for P275NH after manufacturing?
Common inspections: visual inspection (surface defects), ultrasonic testing (internal flaws), radiographic testing (weld quality), tensile testing, impact testing, and hardness testing, complying with EN 10028-2 and customer specifications.
Does P275NH have corrosion resistance? Can it be used in corrosive environments?
P275NH has basic atmospheric corrosion resistance but is not suitable for strong corrosive environments (e.g., acidic/alkaline media). It needs anti-corrosion coatings or linings if used in such harsh conditions to extend service life.